CNCGLASS-Bubbles-After-Vacuum-Bagging-SGP-Glass

This article is a process case on why bubbles can remain in SGP laminated glass after vacuum bagging. The example is a large dual-ply ionoplast plate, about 9.5 square meters, that still showed a wide field of bubbles and haze after the autoclave. The shop found that the autoclave vacuum circuit had lost power, and that the second-stage hold at 125 degrees Celsius was too cool for ionoplast flow. After the hardware was repaired and the second hold was raised to 135 degrees Celsius, a controlled rework cleared the bubbles.

Published by Peter Lin CNC Glass Interlayer www.cncglass.com www.c-n-c.com Mail: cnc@cncglass.com benext77@hotmail.com